Extraction of alumina from Iraqi colored kaolin by lime-sinter process
In this work lime -sinter method was investigated to recover alumina from Iraqi colored kaolinitic claystone. The claystone was intimately mixed with limestone and the mixture was sintered. The annealed sintered material dusts to a fine powder which required no grinding. This material was leached wi...
Gespeichert in:
Veröffentlicht in: | Iraqi Bulletin of Geology and Mining 2014, Vol.10 (3), p.109-117 |
---|---|
Hauptverfasser: | , , , , , |
Format: | Artikel |
Sprache: | ara ; eng |
Online-Zugang: | Volltext |
Tags: |
Tag hinzufügen
Keine Tags, Fügen Sie den ersten Tag hinzu!
|
Zusammenfassung: | In this work lime -sinter method was investigated to recover alumina from Iraqi colored
kaolinitic claystone. The claystone was intimately mixed with limestone and the mixture was
sintered. The annealed sintered material dusts to a fine powder which required no grinding.
This material was leached with sodium carbonate solution, and an alumina extract (sodium
aluminate solution) was obtained. By bubbling carbon dioxide gas into this extract solution,
gibbsite [Al(OH)3] precipitated and on calcinations at 1350 °C ,alumina in the form of alpha
(α – Al2O3) of high purity (98%) can be obtained. In the course of this investigation, the effect
of sintering temperature and time, concentration of sodium carbonate solution, leaching time
and sintered powder to sodium carbonate solution ratio were studied. About 85% of the
alumina in the claystone was extracted at the optimum conditions. The alumina obtained in
this method assaying 98% Al2O3, 1.45% SiO2, 0.04% Fe2O3, and 0.13% CaO and, 0.15%
Na2O |
---|---|