Measurement of Residual Stress in Diamond Films Obtained Using Chemical Vapor Deposition
Diamond films were deposited on a p-type Si substrate using the hot filament chemical vapor deposition (HFCVD) method. Residual stresses in the films were subsequently measured using the curvature, the X-ray diffraction (XRD) sin 2 ψ, and the Raman peak shift methods. Results from the three methods...
Gespeichert in:
Veröffentlicht in: | Japanese Journal of Applied Physics 1998-07, Vol.37 (7B), p.L890 |
---|---|
Hauptverfasser: | , |
Format: | Artikel |
Sprache: | eng |
Online-Zugang: | Volltext |
Tags: |
Tag hinzufügen
Keine Tags, Fügen Sie den ersten Tag hinzu!
|
Zusammenfassung: | Diamond films were deposited on a p-type Si substrate using the hot filament chemical vapor
deposition (HFCVD) method. Residual stresses in the films were subsequently measured using the
curvature, the X-ray diffraction (XRD) sin
2
ψ, and the Raman peak shift methods. Results from the three
methods were in agreement and indicated that residual stresses changed from compressive to tensile with
increasing film thickness, but the maximum or minimum extent of the stresses measured by the Raman
and XRD methods was 3–5 times larger than those by the curvature method. These results were
correlated with the results from the determination of Young's modulus and total peak shifts by the XRD and
the Raman methods. Young's moduli of diamond films were measured by the sonic resonance method,
and the peak shift due to residual stress was separated from the total peak shift using the beam bending
theory. After the adjustment, the disparity among the stress measurements was significantly reduced and a
stress range of -0.5 GPa to +0.5 GPa was obtained. |
---|---|